C5191
ISO N (non-ferrous)Copper alloy (phosphor bronze. Former name: phosphor bronze Class 2, former designation PB×2). Standard: JIS H 3110 (Phosphor bronze and nickel silver sheets, plates and strips) / JIS H 3270 (Beryllium copper, phosphor bronze and nickel silver rods and bars, and wires) (Latest edition year not confirmed).
International equivalents
“Close” means composition or properties are not exactly the same. Before substituting, check the values in each standard.
| System | Designation | Number | Relation | Confidence |
|---|---|---|---|---|
| JIS | C5191 | JIS H 3110 (Phosphor bronze and nickel silver sheets, plates and strips) / JIS H 3270 (Beryllium copper, phosphor bronze and nickel silver rods and bars, and wires) | — | |
| ASTM/UNS | C51900Phosphor Bronze 6% | UNS C51900 | Equivalent (same row in the cross-reference table; lower limit of Sn differs) | Agrees in 2+ sources[6][9][4] |
| EN | CuSn6 | CW452K | Equivalent (same row in the cross-reference table; lower limit of P and impurity limits differ) | Agrees in 2+ sources[9][7][10][8][11] |
| GB | QSn6.5-0.1Ningbo Jintian's C51900 page) / QSn7-0.2 (the same company's C5191 page | close | One source / reference[12][4] |
Differences between the equivalents (from the sources)
- ASTM/UNS C51900: The heading of Poongsan's C5191 page is "C5191 Phosphor Bronze (PB2), UNS No. C51900", with composition Sn 5.0–7.0 and P 0.03–0.35 (lower limits lower than JIS Sn 5.5–7.0). Aurubis's US-market document lists "UNS C51900, EN CW452K, JIS C5191" as comparison standards (its own composition is Sn 5.5–7.0, P 0.03–0.18, Zn ≤0.1). Ningbo Jintian's C5191 page also lists UNS C51900
- EN CuSn6: Aurubis places it in the same row as JIS C5191. Wieland (B16 and the Ulm plant table), Kemper and Matthey give CuSn6 = CW452K = C51900 (no JIS designation is stated). Matthey's EN composition is Sn 5.50–7.00, P 0.01–0.35, Ni ≤ 0.20, Pb ≤ 0.02, Fe ≤ 0.10, Zn ≤ 0.20, others ≤ 0.20, Cu remainder; Sn is the same as JIS, and the lower limit of P is lower than JIS (0.03). Matthey also lists the old DIN number 2.1020. Note that in Wieland's table JIS C5212 is CuSn8 (CW453K, C52100), a different alloy from C5191
- GB QSn6.5-0.1: The two pages of the same company, Ningbo Jintian, disagree. The C51900 page places QSn6.5-0.1 in the same row as C51900, CuSn6 and JIS C5191, with composition Sn 6.0–7.0, P 0.10–0.25 (narrower than JIS). The C5191 page gives QSn7-0.2 (written as GB/T 1176-1987) and states the DIN counterpart as CuSn8 (in Wieland's table CuSn8 is on the C5212 side)
Related specifications (AMS, ASTM etc.)
Specifications called up on purchase orders and drawings. AMS are SAE aerospace material specifications, split by product form (bar, plate, forging), melting practice and heat treatment. Standard texts are paid, so only titles and scopes checked on the publishers’ public pages are shown.
| Spec | Scope | Confidence |
|---|---|---|
| ASTM B103/B103M | Phosphor bronze plate, strip and rolled bar. Wieland gives the tensile strength of C51900 Annealed, H02 and H04 as ASTM B103 values, and Ningbo Jintian cites ASTM B103/B103M-2019. The current edition has not been confirmed | Agrees in 2+ sources[7][12] |
| ASTM B139/B139M | Phosphor bronze rod and bar. Cited by Ningbo Jintian's C51900 and C5191 pages (written as ASTM B139/B139M-2013). One company only | One source / reference[12][4] |
All ASTM standards on Kezuriba: ASTM standards quick reference · AMS specifications quick reference.
Chemical composition (mass %)
As specified in JIS (Japan Copper and Brass Association composition table / Japan Copper Development Association pamphlet)
| Element | Range | Confidence |
|---|---|---|
| Sn | 5.5 – 7.0 | Agrees in 2+ sources[1][2] |
| P | 0.03 – 0.35 | Agrees in 2+ sources[1][2][6] |
| Cu | Balance | Agrees in 2+ sources[2][6] |
| Cu+Sn+P | Total of Cu, Sn and P is 99.5 or more (“Other requirements” column of the Japan Copper and Brass Association table) | One source / reference[1] |
| Pb, Fe, Zn | In the Japan Copper and Brass Association composition table, Pb, Fe and Zn are all “-” (no limit). EN CuSn6 (Matthey) gives Pb ≤ 0.02, Fe ≤ 0.10, Zn ≤ 0.20, Ni ≤ 0.20, and the Ningbo Jintian C5191 page gives Pb ≤ 0.02, Fe ≤ 0.05, Zn ≤ 0.1, so whether the current JIS has impurity limits must be checked in the JIS text itself | One source / reference[1] |
Density
8.8 g/cm³
Wieland B16 (CuSn6) 8.80, Aurubis (C51900) 8.80 and Kemper (CuSn6) 8.8 agree. The specific gravity of Poongsan's C5191 is 8.83, Matthey (CuSn6) 8.82, and Ningbo Jintian 8.80–8.86. JIS does not specify density
Calculate weight in C5191 →Material cost comparison: Metal and plastic price guide.
Mechanical properties
“Reference” values are not specified minimums from the standard but figures published by makers and others.
| Condition | Tensile MPa | Yield MPa | Elong. % | Hardness | Type of value |
|---|---|---|---|---|---|
| Plate and strip: JIS H 3110 specified values (with temper and thickness classes) | — | — | — | — | JIS specified value Not confirmed |
| Rod and wire: JIS H 3270 specified values | — | — | — | — | JIS specified value Not confirmed |
| 1/2H (strip) | 490-610 | ≥ 450 (0.2% proof strength) | ≥ 20 | HV 150-205 | Manufacturer's stated value (Poongsan. The way ranges and lower limits are written suggests JIS specified values, but the material does not say JIS. No thickness condition) One source / reference[6] |
| H (strip) | 590-685 | ≥ 520 (0.2% proof strength) | ≥ 8 | HV 180-230 | Manufacturer's stated value (same as above) One source / reference[6] |
| EH (strip) | 635-720 | ≥ 590 (0.2% proof strength) | ≥ 5 | HV 200-240 | Manufacturer's stated value (same as above) One source / reference[6] |
| CuSn6 (CW452K) R350 (strip, EN temper) | 350-420 | ≤ 300 (0.2% proof strength) | ≥ 45 | HV 80-110 (Wieland, reference) / 90-120 (Kemper) | Reference value (EN-system temper; values for CuSn6 strip from Wieland and Kemper) Agrees in 2+ sources[7][8] |
| CuSn6 (CW452K) R420 (strip, EN temper) | 420-520 | ≥ 360 (Wieland) / >=260 (Kemper) (0.2% proof strength) | ≥ 17 | HV 125-165 | Reference value (same as above) Agrees in 2+ sources[7][8] |
| CuSn6 (CW452K) R500 (strip, EN temper) | 500-590 | ≥ 460 (Wieland) / >=450 (Kemper) (0.2% proof strength) | ≥ 8 | HV 160-190 | Reference value (same as above) Agrees in 2+ sources[7][8] |
| CuSn6 (CW452K) R560 (strip, EN temper) | 560-650 | ≥ 530 (Wieland) / >=500 (Kemper) (0.2% proof strength) | ≥ 5 | HV 180-210 | Reference value (same as above) Agrees in 2+ sources[7][8] |
| CuSn6 (CW452K) R640 (strip, EN temper) | 640-730 | ≥ 610 (Wieland) / >=600 (Kemper) (0.2% proof strength) | ≥ 3 | HV 200-230 | Reference value (same as above) Agrees in 2+ sources[7][8] |
| CuSn6 (CW452K) R720 (strip, EN temper) | ≥ 720 | ≥ 690 (0.2% proof strength) | — | HV 220 or more | Reference value (same as above) Agrees in 2+ sources[7][8] |
| C51900 Annealed / O60 (strip, ASTM B103 temper) | 330-435 (Wieland) / 331-434 (Aurubis, 48-63ksi) | — | — | — | Reference value (tensile strength of C51900 per ASTM B103; given by Wieland and Aurubis) Agrees in 2+ sources[7][9] |
| C51900 H02 (strip, ASTM B103 temper) | 440-545 (Wieland) / 441-545 (Aurubis, 64-79ksi) | — | — | — | Reference value (same as above) Agrees in 2+ sources[7][9] |
| C51900 H04 (strip, ASTM B103 temper) | 550-660 (Wieland) / 552-662 (Aurubis, 80-96ksi) | — | — | — | Reference value (same as above) Agrees in 2+ sources[7][9] |
1 MPa ≈ 145 psi (0.145 ksi). Hardness conversion · unit converter
Machinability notes (as stated in the sources)
- Machinability rating in the Japan Copper and Brass Association / Japan Copper Center pamphlet: phosphor bronze = 20 (leaded brass C3604 = 100; pure copper is also 20)[2]
- Matthey gives the machinability rating of CuSn6 as 20% (basis: CuZn39Pb3 = 100%) and calls it moderate[11]
- Sandvik Coromant defines ISO N as soft non-ferrous metals below 130 HB, and divides lead-free copper alloys as N3.1 (100 HB, specific cutting force 1350 N/mm²) and high-strength bronze above 225 HB as N3.4. Its description of “bronze” is an alloy of Sn 10–14% and Al 3–10%; it does not name Sn 6% phosphor bronze[5]
- Japan Copper Center pamphlet: phosphor bronze has good mechanical strength, spring properties and corrosion resistance, and is non-magnetic. Because of its high mechanical strength and excellent wear resistance, it is also used for gears and bearings. The features of C5102–C5212 are ductility, fatigue resistance and corrosion resistance (suitable for springs) (this is not a statement about machinability)[2]
- Aurubis: cold workability of C51900 is excellent; hot workability is poor[9]
- Poongsan: C5191 has good corrosion resistance to seawater, industrial atmospheres and neutral salt water, and is resistant to stress corrosion cracking[13]
Frequently asked questions about C5191
- What are the international equivalent grades (JIS, ASTM, SAE, EN, ISO, GB) for C5191?
- Comparable grades to C5191 (Copper alloy (phosphor bronze. Former name: phosphor bronze Class 2, former designation PB×2)) include C51900, CuSn6, QSn6.5-0.1. Because composition limits and mechanical property ranges differ slightly between standards, verify the exact table values above before substituting on a drawing.
- What is the ISO material group and specific cutting force (kc1) of C5191?
- C5191 belongs to ISO material group N (non-ferrous). Select insert grades and chipbreakers rated for ISO N.
- What is the most important precaution when machining C5191?
- Machinability rating in the Japan Copper and Brass Association / Japan Copper Center pamphlet: phosphor bronze = 20 (leaded brass C3604 = 100; pure copper is also 20)
Sources
Primary sources (public documents from makers, industry associations and standards bodies), numbered where each value is cited. Many are in Japanese.
- copper-brass.gr.jp https://www.copper-brass.gr.jp/db_access/seibun.htm
- jcda.or.jp https://www.jcda.or.jp/publication/pamphlet/pdf/shindouhin_kaitei_20211130%20(2).pdf#page=…
- jcda.or.jp https://www.jcda.or.jp/publication/pamphlet/pdf/shindouhin_kaitei_20211130%20(2).pdf#page=…
- en.jtcopper.com https://en.jtcopper.com/c5191-bronze.html
- sandvik.coromant.com https://www.sandvik.coromant.com/en-us/knowledge/materials/workpiece-materials
- poongsan.co.kr https://poongsan.co.kr/include/images/cs/%EC%A0%9C%ED%92%88%EA%B8%B0%EC%88%A0%EC%9E%90%EB%…
- wieland.com https://www.wieland.com/pl/content/download/9658/file/B16_global.pdf
- kemper-group.com https://www.kemper-group.com/media/de-at/content/04-produkte/walzprodukte/datenblaetter/cu…
- aurubis.be https://www.aurubis.be/en/dam/jcr:233d5205-94fc-4bf8-99c1-d30fb09d2187/c51900-cusn6-us.pdf
- wieland.com https://www.wieland.com/pl/about/wieland-worldwide/wieland-ulm
- matthey.ch https://www.matthey.ch/fileadmin/user_upload/downloads/fichetechnique/EN/CuSn6_v22E.pdf
- en.jtcopper.com https://en.jtcopper.com/c51900-bronze.html
- poongsan.co.kr https://poongsan.co.kr/include/images/cs/%EC%A0%9C%ED%92%88%EA%B8%B0%EC%88%A0%EC%9E%90%EB%…