Printed from Kezuriba (kezuriba.net/en/materials/sncm439/)
SNCM439
ISO P (steel)Alloy steels for machine structural use (nickel-chromium-molybdenum steel). Standard: JIS G 4053 (JIS G 4053:2016).
International equivalents
“Close” means composition or properties are not exactly the same. Before substituting, check the values in each standard.
| System | Designation | Number | Relation | Confidence |
|---|---|---|---|---|
| JIS | SNCM439 | JIS G 4053 | — | |
| AISI/SAE | 4340 | UNS G43400 | close | Agrees in 2+ sources[6][5][3] |
| EN | 41NiCrMo7-3-2 | 1.6563 | close | One source / reference[5] |
| DIN | 40NiCrMo6designation of the former DIN | close | One source / reference[6] | |
| GB | 40CrNiMoAKyocera) / 40CrNi2Mo (Sumitomo Electric | close | One source / reference[6][5][7] |
Differences between the equivalents (from the sources)
- AISI/SAE 4340: Kyocera's metal material symbol cross-reference table (4340 in the SNCM439 row) and Sumitomo Electric's metal material symbol cross-reference table (4340 in the AISI/ASTM column of the SNCM439 row) agree. The UNS number is from the SAE standards table in the Nippon Steel "Bars and Wire Rods" catalog (4340 = G43400). However, Sumitomo Electric also places 4340 in the SNCM447 row. Compared with the aircraft-grade 4340 (AMS 6414/6415: C 0.38–0.43, Mn 0.65–0.90, Ni 1.65–2.00, Cr 0.70–0.90, Mo 0.20–0.30) given on the AISI 4340 material page, SNCM439 has wider ranges: C lower limit 0.36, Ni lower limit 1.60, Cr 0.60–1.00, Mo lower limit 0.15. The general 4340 composition in SAE J404 is not confirmed in primary sources
- EN 41NiCrMo7-3-2: DIN/EN column of Sumitomo Electric's comparison table (the same designation in both the SNCM439 and SNCM447 rows). The composition of this grade and which EN/ISO standard it appears in are not confirmed in primary sources
- DIN 40NiCrMo6: DIN column of Kyocera's comparison table (SNCM439 row). The material number and whether it remains in the current EN standards are not confirmed in primary sources. The designation conflicts with Sumitomo Electric (41NiCrMo7-3-2)
- GB 40CrNiMoA: The GB column of the SNCM439 row differs: 40CrNiMoA at Kyocera and 40CrNi2Mo at Sumitomo Electric. Mitsubishi Materials' comparison table places 40CrNiMoA in the row of 34CrNiMo6 and AISI 4340 (JIS column blank). The GB composition could not be obtained from primary sources
Related specifications (AMS, ASTM etc.)
Specifications called up on purchase orders and drawings. AMS are SAE aerospace material specifications, split by product form (bar, plate, forging), melting practice and heat treatment. Standard texts are paid, so only titles and scopes checked on the publishers’ public pages are shown.
| Spec | Scope | Confidence |
|---|---|---|
| JIS G 3509-1 | SNCM439RCH is available as wire rod for cold heading (list of grades in the Kobe Steel standard table). The table notes state that the lower limit of Si may be set below 0.15% by agreement, Al may be added by agreement for grain refinement, and the impurity Cu is 0.30% or less | One source / reference[1] |
All ASTM standards on Kezuriba: ASTM standards quick reference · AMS specifications quick reference.
Chemical composition (mass %)
As specified in JIS G 4053
| Element | Range | Confidence |
|---|---|---|
| C | 0.36 – 0.43 | Agrees in 2+ sources[1][2] |
| Si | 0.15 – 0.35 | Agrees in 2+ sources[1][2] |
| Mn | 0.6 – 0.9 | Agrees in 2+ sources[1][2] |
| P | ≤ 0.03 | Agrees in 2+ sources[1][2] |
| S | ≤ 0.03 | Agrees in 2+ sources[1][2] |
| Ni | 1.6 – 2.0 | Agrees in 2+ sources[1][2] |
| Cr | 0.6 – 1.0 | Agrees in 2+ sources[1][2] |
| Mo | 0.15 – 0.30 | Agrees in 2+ sources[1][2] |
| Cu | ≤ 0.3 | Agrees in 2+ sources[1][2] |
Density
—
Not confirmed
No density for SNCM439 was found in Japanese primary sources. For reference: for AISI 4340, a close grade, its material page gives 7.84 (Latrobe, now Carpenter; MIL-HDBK-5J). The SIJ datasheet for 34CrNiMo6 also gives 7.84, but many sources assign 34CrNiMo6 to SNCM447 (see the equivalents note below), so it is not adopted as the SNCM439 value (same treatment as SCM435 and SCM440)
The density could not be confirmed. In the weight calculator, use “Steel, general value” or enter your own.
Material cost comparison: Metal and plastic price guide.
Mechanical properties
“Reference” values are not specified minimums from the standard but figures published by makers and others.
| Condition | Tensile MPa | Yield MPa | Elong. % | Hardness | Type of value |
|---|---|---|---|---|---|
| Quenched and tempered (quenched 820–870°C oil cool / tempered 580–680°C rapid cool) | ≥ 980 | ≥ 885 | ≥ 16 | HB 293-352 | Reference values (manufacturers' "(Reference) Material data examples of alloy steels for machine structural use" tables; not JIS specified values). Tensile tested with No. 4 test piece, impact with 2 mm U-notch. Sanyo Special Steel explains that "these are values for a 25 mm diameter test piece properly quenched and tempered, and cannot be guaranteed for thicker steel". The hardness symbol is HBW at Kobe Steel and HB at Sanyo Agrees in 2+ sources[1][2] |
| Annealed about 820°C furnace cool, or about 670°C air cool (furnace cool) | — | — | — | HB 217-269 | Reference value (Sanyo Special Steel; the table marks it as a reference value) One source / reference[2] |
1 MPa ≈ 145 psi (0.145 ksi). Hardness conversion · unit converter
Machinability notes (as stated in the sources)
- Sandvik Coromant states that the machinability of low-alloy steels is determined by alloy content and heat treatment (hardness). SNCM439 is a tough steel used quenched and tempered, and even in the manufacturers' reference values, at HB 293–352 it is about as hard as SCM440 (HB 285–352) or slightly harder[4][1]
- In Sanyo Special Steel's reference values, even after annealing the hardness is HB 217–269, harder than SCM440 (HB 179–217). In addition to annealing at about 820°C with furnace cooling, a method of holding at about 670°C (below the transformation point) and then air or furnace cooling is also listed (for SNCM625, 630, and 616 the company explains that "ordinary annealing does not soften them sufficiently, so after normalizing, hold at about 670°C and air or furnace cool"; no such explanation is given for SNCM439)[2]
Frequently asked questions about SNCM439
- What are the international equivalent grades (JIS, ASTM, SAE, EN, ISO, GB) for SNCM439?
- Comparable grades to SNCM439 (Alloy steels for machine structural use (nickel-chromium-molybdenum steel)) include AISI 4340, 41NiCrMo7-3-2, 40NiCrMo6, 40CrNiMoA. Because composition limits and mechanical property ranges differ slightly between standards, verify the exact table values above before substituting on a drawing.
- What is the ISO material group and specific cutting force (kc1) of SNCM439?
- SNCM439 belongs to ISO material group P (steel). Select insert grades and chipbreakers rated for ISO P.
- What is the most important precaution when machining SNCM439?
- Sandvik Coromant states that the machinability of low-alloy steels is determined by alloy content and heat treatment (hardness). SNCM439 is a tough steel used quenched and tempered, and even in the manufacturers' reference values, at HB 293–352 it is about as hard as SCM440 (HB 285–352) or slightly harder
Sources
Primary sources (public documents from makers, industry associations and standards bodies), numbered where each value is cited. Many are in Japanese.
- kobelco.co.jp https://www.kobelco.co.jp/products/steel-aluminum/wirerod/pdf/202012_wirerod_standard.pdf
- sanyo-steel.co.jp https://www.sanyo-steel.co.jp/product/special_steel/images/pdf/akahon_201906.pdf
- nipponsteel.com https://www.nipponsteel.com/product/catalog_download/__icsFiles/afieldfile/2026/04/23/B001…
- sandvik.coromant.com https://www.sandvik.coromant.com/en-us/knowledge/materials/workpiece-materials
- sumitool.com https://www.sumitool.com/downloads/cutting-tools/general-catalog/assets/pdf/n2.pdf
- kyocera.co.jp https://www.kyocera.co.jp/prdct/tool/wp-content/uploads/2016/06/R_2016.pdf
- mitsubishicarbide.net https://www.mitsubishicarbide.net/contents/mhg/ru/manual/material_cross_reference.pdf